This paint is an exterior paint made of selected high-grade acrylic emulsion and pigment with excellent weather resistance. In particular, it is an economical paint suitable for large construction projects due to its excellent hiding power, weather resistance, water resistance, and alkali resistance, and superb painting workability. Additionally, it is an exterior water-based paint widely used for new buildings (e.g., cement mortar, concrete, P.C, plaster, etc.) or for repair painting.
Surface treatment ;
1. The material should be sufficiently cured (cured more than 30 days at 20℃)
2. Laitance, dust, oil and other contaminants on the surface must be completely removed.
3. The proper pH of the material must be less than 9, and the percentage of moisture content must be less than 6%.
4. The gaps and grooves on the surface must be filled with exterior water-based putty, and surface adjustment should be made before coating.
Coating method :
1. Primer
① After surface treatment, dilute the water-based permeable sealer DNX-4001 with water up to 100%, and apply once at a dry film thickness of 15㎛ with a roller or brush.
② For areas where the absorption of the surface is severe, apply once more coating.
2. Top Coat
① After at least 3 hours at 20℃ following undercoating, apply this paint twice to get a dry film thickness of 60㎛ with a brush, roller or spray.
② At this time, apply by diluting with water up to 20%.
③ After 2 coats, the re-coating interval is at least 3 hours after the first top coating at 20℃.
This paint is an exterior paint made of selected high-grade acrylic emulsion and pigment with excellent weather resistance. In particular, it is an economical paint suitable for large construction projects due to its excellent hiding power, weather resistance, water resistance, and alkali resistance, and superb painting workability. Additionally, it is an exterior water-based paint widely used for new buildings (e.g., cement mortar, concrete, P.C, plaster, etc.) or for repair painting.
Surface treatment ;
1. The material should be sufficiently cured (cured more than 30 days at 20℃)
2. Laitance, dust, oil and other contaminants on the surface must be completely removed.
3. The proper pH of the material must be less than 9, and the percentage of moisture content must be less than 6%.
4. The gaps and grooves on the surface must be filled with exterior water-based putty, and surface adjustment should be made before coating.
Coating method :
1. Primer
① After surface treatment, dilute the water-based permeable sealer DNX-4001 with water up to 100%, and apply once at a dry film thickness of 15㎛ with a roller or brush.
② For areas where the absorption of the surface is severe, apply once more coating.
2. Top Coat
① After at least 3 hours at 20℃ following undercoating, apply this paint twice to get a dry film thickness of 60㎛ with a brush, roller or spray.
② At this time, apply by diluting with water up to 20%.
③ After 2 coats, the re-coating interval is at least 3 hours after the first top coating at 20℃.
This paint is an exterior paint made of selected high-grade acrylic emulsion and pigment with excellent weather resistance. In particular, it is an economical paint suitable for large construction projects due to its excellent hiding power, weather resistance, water resistance, and alkali resistance, and superb painting workability. Additionally, it is an exterior water-based paint widely used for new buildings (e.g., cement mortar, concrete, P.C, plaster, etc.) or for repair painting.
Surface treatment ;
1. The material should be sufficiently cured (cured more than 30 days at 20℃)
2. Laitance, dust, oil and other contaminants on the surface must be completely removed.
3. The proper pH of the material must be less than 9, and the percentage of moisture content must be less than 6%.
4. The gaps and grooves on the surface must be filled with exterior water-based putty, and surface adjustment should be made before coating.
Coating method :
1. Primer
① After surface treatment, dilute the water-based permeable sealer DNX-4001 with water up to 100%, and apply once at a dry film thickness of 15㎛ with a roller or brush.
② For areas where the absorption of the surface is severe, apply once more coating.
2. Top Coat
① After at least 3 hours at 20℃ following undercoating, apply this paint twice to get a dry film thickness of 60㎛ with a brush, roller or spray.
② At this time, apply by diluting with water up to 20%.
③ After 2 coats, the re-coating interval is at least 3 hours after the first top coating at 20℃.